It’s the machinists in the shop that get a first sense of “Something is Different” or “Something Changed” when a new batch of material is put into production. In my experience, these are the five things to check to confirm that it is a purchasing/ supplier issue rather than the machining process out in the shop.

  1. Different Supplier
  2. Different Process
  3. Different Than Ordered
  4. Different Deoxidation
  5. For Machining- Significantly Different Sulfur

Different Supplier-Different suppliers can have different processes, recipes, standards, and practices. Changing or mixing suppliers can induce more variability in a process than an out of control operator in the shop.
Different Process-Maybe it is the same supplier- company, or location. but perhaps they can make the product on two or more different process lines. maybe one from a coil to bar, the other from bar to bar. Maybe the straightners are different.
Different Than You Ordered-Maybe you ordered Cold Drawn and they supplied you with Cold Finished. In Cold Drawing, the cold work of die drawing adds strain which changes the material’s mechanical properties. Cold Finished could include cold drawing, but often means hot roll that has been turned and polished to get the same tolerance and surface finish, but does nothing to change the material’s mechanical properties.
Different Deoxidation-Maybe you ordered aluminum fine grain, and they supplied Vanadium. Maybe you wanted Silicon .10 max coarse grain practice, and the only steel in stock was .15-.35 silicon killed and your purchasing department said, “Yeah, we’ll take it.” Different deoxidation can affect mechanical properties too.
For Machining-Significantly Different Sulfur Levels-There are several “tipping points”  for sulfur in the non- free-machining grades of carbon and alloy steels. Steels showing a Sulfur analysis of 0.020% minimum never were submitted to me for machining claims in over 20 years of managing labs and claims in my steel mill career. Steels below 0.018% would often be sent back, especially in plain medium carbon grades like 1045 and 1050.  Typically the customer would complain about fighting it to get production.
Steels below 0.015% Sulfur would almost always elicit a very heightened urgency from the customer who couldn’t keep tools in the machine and couldn’t get finish. Steels below 0.010% almost always got a call from their VP to our VP who then put me on the case. This is especially true in medium carbon alloy grades (4140 etc.) where the material is challenging anyhow, especially on screw machines.
I had one claim once upon a time for a batch of 4140 with 0.003% Sulfur. The guys in the shop called it “Toolproof.”
So these are five quick items to check on the material certs to see of the unexpected variability  you are encountering in the shop might, just might, be the result of supply chain changes upstream of your screw machines.
(Note: My experience was primarily supplying the shops running high volumes on cam automatic screw machines. Even with carbides, coatings and cnc controls, the 5 items listed above can make a serious difference in your shop’s performance.)

Leave a Reply

Your email address will not be published. Required fields are marked *

You may use these HTML tags and attributes:

<a href="" title=""> <abbr title=""> <acronym title=""> <b> <blockquote cite=""> <cite> <code> <del datetime=""> <em> <i> <q cite=""> <s> <strike> <strong>